A distributor takes delivery of twelve pallets in June, stacks them in a warehouse corner, and ships them out in November. When the first container is unpacked, a share of the blocks read below 12.2 V and fail the incoming check. The batteries were not defective. They were never measured, never topped up, and never rotated. Self-discharge is slow and invisible, which is exactly why it costs money.
This is a working procedure for warehouse teams and wholesale buyers: how to measure, what each voltage level means, which recharge profile to apply, and how to turn a log into a real interval instead of a guess. It ends with block sizes for pallet planning.
Every charged lead-acid block loses a small share of its capacity per month through internal self-discharge. The rate is not constant. It roughly doubles for each 10 °C rise in ambient temperature, so a rack under a metal roof in summer behaves nothing like the same rack in a shaded aisle in winter. Add slow sulphation on the plates and the loss stops being recoverable: a block left at low state of charge for long enough will not return to rated capacity after a normal charge.
Two consequences for purchasing. First, stock age matters as much as the model, so ask for the date code on the pallet label, not only on the invoice. Second, the unit behind a warranty claim is often the one that sat at the back of the rack, not the one that was worked hard.
| Open-circuit voltage, 12 V block at 25 °C | Reading | Action |
|---|---|---|
| 12.70 V or above | Above the recharge line | Log, return to stock, recheck at the next cycle |
| 12.50 to 12.69 V | Drifting | Top-up charge within 30 days |
| 12.20 to 12.49 V | Low | Charge before dispatch, do not ship as found |
| Below 12.20 V | Out of range | Quarantine, capacity check, then decide under your return policy |
These lines are a starting set for a 12 V VRLA block. Correct them with your own log as soon as three months of readings exist.
A top-up is not a full charge. For CHISEN 6-DZF and 6-DMF blocks the recommended constant-voltage stage is 14.7 to 14.9 V per 12 V block (14.8 V typical), with current limited to 0.25 to 0.30 I2 (0.28 I2 typical), and temperature compensation of about −3.0 mV per °C per block away from 25 °C. A charger that only reaches 13.8 V will take days and still leave a drifted block short. Charge in a ventilated area, follow local rules for the installation, and have the work done by qualified personnel.
Do not copy an interval from a catalogue; derive it. If a pallet logs 12.78 V in July and 12.68 V in August at 28 °C ambient, the block is losing about 0.10 V per month. The distance to the 12.50 V action line is 0.28 V, which at that rate is 2.8 months. Set the recheck at 60 days and keep roughly one month of buffer, then shorten it if the summer aisle runs hotter than the log suggests.
Before your own data exists, this is a reasonable planning default:
| Average aisle temperature | Inspection and top-up interval |
|---|---|
| 20 °C and below | 120 days |
| 21 to 30 °C | 90 days |
| 31 to 40 °C | 45 days |
| Above 40 °C | 30 days, plus forced ventilation |
These are inspection intervals, not a storage warranty. They are a planning default that your voltage log should overrule as soon as it disagrees.
One pallet of 6-DZF-20 blocks holds 60 units. Measuring one block takes about 45 seconds with the log entry, so a full pallet is about 45 minutes per cycle, and twelve pallets is around nine hours a year. Those are example assumptions for labour planning, not a quotation. Compare that with a returned container, a credit note and freight both ways.
| Model | Capacity | Dimensions | Weight range | Terminal |
|---|---|---|---|---|
| 6-DZF-12 | 12 V 12 Ah | 151 x 99 x 99 mm | 3.60 to 4.20 kg, four grades | Φ8.0-M5 |
| 6-DZF-20 | 12 V 20 Ah | 180 x 76 x 170 mm, some grades 183 x 78 x 170 mm | 6.10 to 7.00 kg, six grades | Φ8.8-M5 |
| 6-DMF-32, case type A | 12 V 32 Ah | 267 x 78 x 170 mm | 9.10 to 10.40 kg, three grades | Φ8.8-M5 |
| 6-DMF-32, case type B | 12 V 32 Ah | 224 x 93 x 175 mm | 9.20 kg | Φ9.8-M5 |
Weight and dimensions come in grades, so confirm the grade on the packing list before a pallet drawing is printed. The 6-DMF-32 exists in two case types, A and B, with different footprints and terminals; state which case the vehicle frame accepts before the order is placed.
The DZF and DMF series are produced and tested to GB/T 22199.1-2025 and T/ZJXDC 001-2021. Factory test data at 25 °C shows more than 360 cycles in normal use and more than 650 cycles with proper maintenance. Those figures are test data, not a field specification: duty cycle, depth of discharge and the recharge routine move the result.
Send the pallet count, the aisle temperature in the hottest month, monthly outbound volume, and the model or case type you need. We reply with a mixed-pallet plan for wholesale or OEM orders, sample blocks for your own bench test, and the test report list for the model you select. OEM orders can carry your label; ask for the sample sheet and the packing drawing in the same message so label position and pallet layout are fixed before production. CHISEN Battery supplies the DZF, DMF and EVF series from ZHEJIANG CHISEN BATTERY CO.,LTD to distributors and fleet operators.